Research Article Bond strength of self-adhesive resin cements to composite submitted to different surface pretreatments
Victor Hugo dos Santos1, Sandro Griza2, Rafael Ratto de Moraes3, André Luis Faria-e-Silva1
2014;39(1):-16.
DOI: https://doi.org/10.5395/rde.2014.39.1.12
Published online: January 20, 2014

1Department of Dentistry, Federal University of Sergipe, Aracaju, SE, Brazil.

2Department of Materials Science and Engineering, Federal University of Sergipe, São Cristóvão, SE, Brazil.

3Department of Restorative Dentistry, School of Dentistry, Federal University of Pelotas, Pelotas, RS, Brazil.

Correspondence to André Luis Faria-e-Silva, DDS, MD, PHD. Professor, Departamento de Odontologia, Campus da Saúde, Universidade Federal de Sergipe, Rua Cláudio Batista, s/n - Sanatório, Aracaju-SE, Brazil 49060-100. TEL, +55-79-2105-1824; FAX, +55-79-2105-1822; fariaesilva.andre@gmail.com
• Received: August 25, 2013   • Accepted: November 22, 2013

©Copyights 2014. The Korean Academy of Conservative Dentistry.

This is an Open Access article distributed under the terms of the Creative Commons Attribution Non-Commercial License (http://creativecommons.org/licenses/by-nc/3.0/) which permits unrestricted non-commercial use, distribution, and reproduction in any medium, provided the original work is properly cited.

  • 234 Views
  • 2 Download
  • 21 Crossref
prev next
  • Objectives
    Extensively destroyed teeth are commonly restored with composite resin before cavity preparation for indirect restorations. The longevity of the restoration can be related to the proper bonding of the resin cement to the composite. This study aimed to evaluate the microshear bond strength of two self-adhesive resin cements to composite resin.
  • Materials and Methods
    Composite discs were subject to one of six different surface pretreatments: none (control), 35% phosphoric acid etching for 30 seconds (PA), application of silane (silane), PA + silane, PA + adhesive, or PA + silane + adhesive (n = 6). A silicone mold containing a cylindrical orifice (1 mm2 diameter) was placed over the composite resin. RelyX Unicem (3M ESPE) or BisCem (Bisco Inc.) self-adhesive resin cement was inserted into the orifices and light-cured. Self-adhesive cement cylinders were submitted to shear loading. Data were analyzed by two-way ANOVA and Tukey's test (p < 0.05).
  • Results
    Independent of the cement used, the PA + Silane + Adhesive group showed higher microshear bond strength than those of the PA and PA + Silane groups. There was no difference among the other treatments. Unicem presented higher bond strength than BisCem for all experimental conditions.
  • Conclusions
    Pretreatments of the composite resin surface might have an effect on the bond strength of self-adhesive resin cements to this substrate.
Improvements in adhesive luting systems and ceramic materials have resulted in more conservative tooth preparation procedures for the retention of indirect restorations. Conservative tooth preparations may require luting materials with improved adhesive ability for the retention of restorations.1,2 For many years, adhesive systems have been applied with resin-based luting agents to lute metal-free indirect restorations. However, multistep luting protocols increase the technique sensitivity and clinical time.3-7 Simplified luting agents are gaining increased popularity in this scenario.
Self-adhesive resin cements (SARCs) have been marketed to simplify the clinical procedures and overcome the technique sensitivity of multistep luting systems. According to manufacturers, SARCs do not require pretreatment and their application is accomplished using a single clinical step. Several studies have evaluated the bonding ability of SARCs to dental tissues, with results generally depending on the materials tested.8-11 However, the presence of extensively destroyed coronal structures is relatively common in the clinical setting, requiring the preparation of a composite restoration (core) to serve as an abutment. Fiber posts can be required to retain the core, which is usually built-up using composite resin.12 Therefore, the retention of indirect restorations is dependent on the bonding of the resin cement to the composite core.
Several surface pretreatment protocols have been evaluated to improve the bond strength of repairing composite resin to old one after acid-etching and silane application.13-16 The results of these previous studies indicate that composite pretreatments might improve the repair bond strengths. Treating the composite surface before luting procedures could also enhance the bonding of SARCs to composite cores. However, few studies have evaluated the bonding of SARCs to composite resins. Thus, the aim of this study was to evaluate the effect of different surface treatments of composite resin on the bond strength of SARCs to this substrate. The hypothesis tested was that treating the composite surface would improve the bonding potential of the SARCs.
This in vitro study involved a 2 × 6 factorial design (n = 6 per group). The factors under evaluation were: resin cement (2 levels) and composite pre-treatment (6 levels). The SARCs tested were RelyX Unicem clicker (3M ESPE, St. Paul, MN, USA) and BisCem (Bisco INC., Schaumburg, IL, USA). Table 1 depicts the luting agent compositions. The SARCs were bonded to composite resin discs (2 mm height, 6 mm diameter) of Tetric Ceram (shade B3, Ivoclar Vivadent, Schaan, Liechtenstein). The response variables were microshear bond strength (MPa) to composite and failure mode.
Table 1
Composition of the self-adhesive resin cements tested

*As provided by the manufacturers.

rde-39-12-i001.jpg Download Table Download Table
A total of 72 composite resin discs was prepared by inserting the material into a metallic mold, which was covered with a polyester strip. The composite was inserted using a bulk increment and light-cured for 45 s using a light-emitting diode unit (Radii Cal, SDI, Bayswater, Victoria, Australia) with 800-mW/cm2 irradiance. After light-curing, the discs were removed and embedded in acrylic resin (Jet, Clássico, São Paulo, SP, Brazil), leaving one of the surfaces exposed. After storage in water at 37℃ for 7 days in an incubator (Marconi, Piracicaba, SP, Brazil), the exposed composite resin surface received one of following pretreatments (12 discs per treatment):
  • Control: No surface treatment was performed.

  • Phosphoric acid (PA): The surface was etched with 35% PA (3M ESPE) for 15 seconds, rinsed with water for 10 seconds, and air-dried using compressed air for 10 seconds.

  • Silane: A layer of a silane-coupling agent (RelyX Ceramic Primer, 3M ESPE) was applied and left undisturbed for 60 seconds, and then gently air-dried for 10 seconds.

  • PA + Silane: 35% PA was applied, and the silane agent was applied after the procedures described for the PA group.

  • PA + Adhesive: The non-solvated unfilled resin of the Scotchbond Multipurpose Plus system (3M ESPE,) was applied after acid-etching.

  • PA + Silane + Adhesive: The composite surface was acid-etched, cleaned, and silanized before application of the unfilled resin.

To obtain resin cement cylinders for shear testing, elastomer molds with internal cylindrical orifices (1 mm diameter, 2 mm height) were placed over the prepared surfaces of the composite resin. The unfilled resin was photoactivated for 20 seconds (when applicable) only after positioning of the elastomer molds. The two pastes of each SARC were mixed for 10 seconds, and the mixed cement was inserted into the mold using a dental explorer. Light activation was performed for 20 seconds, the molds were removed, and the specimens were stored in 100% relative humidity. Six composite discs were used for each resin cement-composite pretreatment condition.
After 24 hours, a microshear bond test was conducted on a mechanical testing machine (Instron 5940, Instron, Canton, MA, USA). A thin steel wire (0.2 mm diameter) was looped around each cylinder and aligned with the bonded interface. A shear load was applied to the base of the cylinder at a crosshead speed of 0.5 mm/min until failure. The average value of three bonded cylinders for each composite disc was recorded as the microshear bond strength (MPa) for each composite disc. Data passed the normality (p = 0.097) and equal variance (p = 0.067) tests, and therefore were statistically analyzed using two-way ANOVA (resin cement × composite pretreatment) and Tukey's post hoc test (p < 0.05) using the software SigmaStat 3.5 (Systat Software, Erkrath, Germany).
Results for bond strength are shown in Table 2. The factors "resin cement" (p < 0.001) and "composite pretreatment" (p = 0.009) were both significant, whereas the interaction between the two factors was not significant (p = 0.105). The PA + Silane + Adhesive group showed significantly higher microshear bond strength than the PA and PA + Silane groups. There were no differences among the other surface pretreatments. Unicem showed a higher microshear bond strength than BisCem (p < 0.001), irrespective of the composite pretreatment used. A predominance (above 90%) of adhesive failures was observed regardless of the surface treatment or cement tested.
Table 2
Means (standard deviations) for microshear bond strength, MPa

Distinct lowercase letters in the same column indicate differences between pre-treatments; distinct uppercase letters in the same line indicate differences between resin cements (p < 0.05).

rde-39-12-i002.jpg Download Table Download Table
One of the main bonding mechanisms of SARCs to dental tissues is related to the reaction between the acidic monomers of the cement with calcium present in the dentin and enamel, as SARCs present limited ability to produce an effective hybrid layer.17-20 However, the chemical reaction is limited when SARCs are bonded to the composite resin used as a core. Additionally, the chemical reaction between SARCs and dental calcium aids in buffering the pH of the cement and improves its mechanical properties.21,22 Theoretically, chemical bonding between methacrylate monomers is the main bonding mechanism between SARCs and composite resin. However, there is a reduced amount of unreacted monomers on the surface of cured composite resin to react with the cement.13,14 In the present study, no pretreatment of the composite surface was able to improve the bond strength of the SARCs, although there were differences among the pretreatments evaluated. The tested hypothesis was, therefore, rejected.
An important observation of this study was that the effect of the pretreatments was similar for both SARCs evaluated. Surface etching with PA is commonly used in repair procedures of composite resin restorations, although in some studies, etching with PA was unable to promote a significant increase in microretention on the composite surface.14,15 Acid etching primarily serves to clean the composite surface, resulting in improved surface energy.16 Despite the possibly increased wetting of the SARCs on the cleaned composite surface, etching with PA did not provide higher bonding potential compared to the control.
SARCs present an acidic character in the initial moments after mixing.18 This low pH is important for proper etching of the dental tissues.17 Reaction of the acidic methacrylates with the alkaline ions leached from the acid-soluble glass particles present in SARCs also aids the materials in becoming more hydrophobic with time.18 The pH-buffering effect is important to permit adequate free-radical polymerization of the SARCs and to improve their mechanical stability. Acid-etched surfaces may present residual acidity, which could impair both pH buffering and cement polymerization. Thus, a possible benefit of better wetting after acid etching could be counterbalanced by the reduced mechanical properties of the cement.21,23
Another surface pretreatment evaluated in this study was the use of silane-coupling agent. Silanes promote chemical bonding between inorganic surfaces and polymeric molecules.24 Inorganic fillers in the composite resin are bonded to the organic matrix monomers by silanes, and exposure of the fillers would allow chemical coupling with the glass particles. In the present study, the use of silane was unable to improve the bonding of either SARC to the composite resin. The low availability of exposed glass particles on the composite surface was most likely responsible for those findings. The use of silane after acid-etching also did not alter the bond strength compared to the control group. It has been demonstrated that etching with PA might enhance the reactivity between silica surfaces and silane-coupling agents.25,26 The absence of a significant effect in the present study demonstrates that the acid-etching protocol used was unable to expose the glass particles on the composite surface effectively, thereby impairing the chemical coupling through silanization.
The group with adhesive application after acid etching and silanization showed the highest bond strength values, with significant differences compared with use of PA alone or PA + silane. In contrast, application of adhesive alone did not show significant differences from the other treatments. A possible explanation is that the combined use of silane and adhesive improved the wetting of the adhesive on the composite resin, whereas a possible negative effect of residual acidity did not affect the polymerization of the adhesive. Irrespective of the surface pretreatment performed, Unicem showed higher bond strength than BisCem. Other studies reported similar results when bonding SARCs to tooth tissues and ceramics.10,11,26 Unicem has a higher pH-neutralization ability than BisCem, improving its mechanical properties.21,22
The present results indicate that different pretreatments of the composite resin surface may have distinct effects on the bonding potential of SARCs. However, no pretreatment evaluated was able to improve the bond strength to composite resin as compared with the control surfaces. Other surface treatments used to improve the bonding to cured composite surfaces should be evaluated in future studies, such as the use of alumina sandblasting or etching with hydrofluoric acid.
Within the limitations of the present study, surface treatments might have an effect on the bonding of SARCs to composites.
V.H.S. is grateful to FAPITEC/SE, Brazil for a scholarship.

No potential conflict of interest relevant to this article was reported.

Table 1
Composition of the self-adhesive resin cements tested

*As provided by the manufacturers.

rde-39-12-i001.jpg
Table 2
Means (standard deviations) for microshear bond strength, MPa

Distinct lowercase letters in the same column indicate differences between pre-treatments; distinct uppercase letters in the same line indicate differences between resin cements (p < 0.05).

rde-39-12-i002.jpg
  • 1. Tsitrou EA, van Noort R. Minimal preparation designs for single posterior indirect prostheses with the use of the Cerec system. Int J Comput Dent 2008;11:227-240.PubMed
  • 2. Dietschi D, Argente A. A comprehensive and conservative approach for the restoration of abrasion and erosion. part II: clinical procedures and case report. Eur J Esthet Dent 2011;6:142-159.PubMed
  • 3. Takahashi R, Nikaido T, Ariyoshi M, Kitayama S, Sadr A, Foxton RM, Tagami J. Thin resin coating by dual-application of all-in-one adhesives improves dentin bond strength of resin cements for indirect restorations. Dent Mater J 2010;29:615-622.ArticlePubMed
  • 4. Unlu N, Gunal S, Ulker M, Ozer F, Blatz MB. Influence of operator experience on in vitro bond strength of dentin adhesives. J Adhes Dent 2012;14:223-227.PubMed
  • 5. Gomes GM, Gomes OM, Reis A, Gomes JC, Loguercio AD, Calixto AL. Effect of operator experience on the outcome of fiber post cementation with different resin cements. Oper Dent 2013;38:555-564.ArticlePubMedPDF
  • 6. Pfeifer C, Shih D, Braga RR. Compatibility of dental adhesives and dual-cure cements. Am J Dent 2003;16:235-238.PubMed
  • 7. Kanehira M, Finger WJ, Hoffmann M, Komatsu M. Compatibility between an all-in-one self-etching adhesive and a dual-cured resin luting cement. J Adhes Dent 2006;8:229-232.PubMed
  • 8. Broyles AC, Pavan S, Bedran-Russo AK. Effect of dentin surface modification on the microtensile bond strength of self-adhesive resin cements. J Prosthodont 2013;22:59-62.ArticlePubMed
  • 9. Stona P, Borges GA, Montes MA, Júnior LH, Weber JB, Spohr AM. Effect of polyacrylic acid on the interface and bond strength of self-adhesive resin cements to dentin. J Adhes Dent 2013;15:221-227.PubMed
  • 10. Lisboa DS, Santos SV, Griza S, Rodrigues JL, Faria-e-Silva AL. Dentin deproteinization effect on bond strength of self-adhesive resin cements. Braz Oral Res 2013;27:73-75.ArticlePubMed
  • 11. Faria-e-Silva AL, Menezes Mde S, Silva FP, Reis GR, Moraes RR. Intra-radicular dentin treatments and retention of fiber posts with self-adhesive resin cements. Braz Oral Res 2013;27:14-19.ArticlePubMed
  • 12. Soares LP, Dias KR, de Vasconcellos AB, Sampaio EM, Street A. Effects of different pretreatments on the bond strength of a dual-cure resin core material to various fiber-reinforced composite posts. Eur J Prosthodont Restor Dent 2012;20:41-47.PubMed
  • 13. Melo MA, Moysés MR, Santos SG, Alcântara CE, Ribeiro JC. Effects of different surface treatments and accelerated artificial aging on the bond strength of composite resin repairs. Braz Oral Res 2011;25:485-491.ArticlePubMed
  • 14. Moncada G, Angel P, Fernandez E, Alonso P, Martin J, Gordan VV. Bond strength evaluation of nanohybrid resin-based composite repair. Gen Dent 2012;60:230-234.PubMed
  • 15. Hannig C, Laubach S, Hahn P, Attin T. Shear bond strength of repaired adhesive filling materials using different repair procedures. J Adhes Dent 2006;8:35-40.PubMed
  • 16. Fawzy AS, El-Askary FS, Amer MA. Effect of surface treatments on the tensile bond strength of repaired water-aged anterior restorative micro-fine hybrid resin composite. J Dent 2008;36:969-976.ArticlePubMed
  • 17. Gerth HU, Dammaschke T, Züchner H, Schäfer E. Chemical analysis and bonding reaction of RelyX Unicem and Bifix composites-a comparative study. Dent Mater 2006;22:934-941.ArticlePubMed
  • 18. Ferracane JL, Stansbury JW, Burke FJ. Self-adhesive resin cements-chemistry, properties and clinical considerations. J Oral Rehabil 2011;38:295-314.ArticlePubMed
  • 19. Monticelli F, Osorio R, Mazzitelli C, Ferrari M, Toledano M. Limited decalcification/diffusion of self-adhesive cements into dentin. J Dent Res 2008;87:974-979.ArticlePubMedPDF
  • 20. Al-Assaf K, Chakmakchi M, Palaghias G, Karanika-Kouma A, Eliades G. Interfacial characteristics of adhesive luting resins and composites with dentine. Dent Mater 2007;23:829-839.ArticlePubMed
  • 21. Zorzin J, Petschelt A, Ebert J, Lohbauer U. pH neutralization and influence on mechanical strength in self-adhesive resin luting agents. Dent Mater 2012;28:672-679.ArticlePubMed
  • 22. Madruga FC, Ogliari FA, Ramos TS, Bueno M, Moraes RR. Calcium hydroxide, pH-neutralization and formulation of model self-adhesive resin cements. Dent Mater 2013;29:413-418.ArticlePubMed
  • 23. Foxton RM, Nakajima M, Hiraishi N, Kitasako Y, Tagami J, Nomura S, Miura H. Relationship between ceramic primer and ceramic surface pH on the bonding of dual-cure resin cement to ceramic. Dent Mater 2003;19:779-789.ArticlePubMed
  • 24. Matinlinna JP, Lassila LV, Ozcan M, Yli-Urpo A, Vallittu PK. An introduction to silanes and their clinical applications in dentistry. Int J Prosthodont 2004;17:155-164.PubMed
  • 25. Loomans BA, Cardoso MV, Roeters FJ, Opdam NJ, De Munck J, Huysmans MC, Van Meerbeek B. Is there one optimal repair technique for all composites? Dent Mater 2011;27:701-709.ArticlePubMed
  • 26. Blatz MB, Phark JH, Ozer F, Mante FK, Saleh N, Bergler M, Sadan A. In vitro comparative bond strength of contemporary self-adhesive resin cements to zirconium oxide ceramic with and without air-particle abrasion. Clin Oral Investig 2010;14:187-192.ArticlePubMedPDF

Tables & Figures

Table 1
Composition of the self-adhesive resin cements tested

*As provided by the manufacturers.

rde-39-12-i001.jpg Download Table Download Table
Table 2
Means (standard deviations) for microshear bond strength, MPa

Distinct lowercase letters in the same column indicate differences between pre-treatments; distinct uppercase letters in the same line indicate differences between resin cements (p < 0.05).

rde-39-12-i002.jpg Download Table Download Table
Table 1
Composition of the self-adhesive resin cements tested

*As provided by the manufacturers.

rde-39-12-i001.jpg
Table 2
Means (standard deviations) for microshear bond strength, MPa

Distinct lowercase letters in the same column indicate differences between pre-treatments; distinct uppercase letters in the same line indicate differences between resin cements (p < 0.05).

rde-39-12-i002.jpg

REFERENCES

  • 1. Tsitrou EA, van Noort R. Minimal preparation designs for single posterior indirect prostheses with the use of the Cerec system. Int J Comput Dent 2008;11:227-240.PubMed
  • 2. Dietschi D, Argente A. A comprehensive and conservative approach for the restoration of abrasion and erosion. part II: clinical procedures and case report. Eur J Esthet Dent 2011;6:142-159.PubMed
  • 3. Takahashi R, Nikaido T, Ariyoshi M, Kitayama S, Sadr A, Foxton RM, Tagami J. Thin resin coating by dual-application of all-in-one adhesives improves dentin bond strength of resin cements for indirect restorations. Dent Mater J 2010;29:615-622.ArticlePubMed
  • 4. Unlu N, Gunal S, Ulker M, Ozer F, Blatz MB. Influence of operator experience on in vitro bond strength of dentin adhesives. J Adhes Dent 2012;14:223-227.PubMed
  • 5. Gomes GM, Gomes OM, Reis A, Gomes JC, Loguercio AD, Calixto AL. Effect of operator experience on the outcome of fiber post cementation with different resin cements. Oper Dent 2013;38:555-564.ArticlePubMedPDF
  • 6. Pfeifer C, Shih D, Braga RR. Compatibility of dental adhesives and dual-cure cements. Am J Dent 2003;16:235-238.PubMed
  • 7. Kanehira M, Finger WJ, Hoffmann M, Komatsu M. Compatibility between an all-in-one self-etching adhesive and a dual-cured resin luting cement. J Adhes Dent 2006;8:229-232.PubMed
  • 8. Broyles AC, Pavan S, Bedran-Russo AK. Effect of dentin surface modification on the microtensile bond strength of self-adhesive resin cements. J Prosthodont 2013;22:59-62.ArticlePubMed
  • 9. Stona P, Borges GA, Montes MA, Júnior LH, Weber JB, Spohr AM. Effect of polyacrylic acid on the interface and bond strength of self-adhesive resin cements to dentin. J Adhes Dent 2013;15:221-227.PubMed
  • 10. Lisboa DS, Santos SV, Griza S, Rodrigues JL, Faria-e-Silva AL. Dentin deproteinization effect on bond strength of self-adhesive resin cements. Braz Oral Res 2013;27:73-75.ArticlePubMed
  • 11. Faria-e-Silva AL, Menezes Mde S, Silva FP, Reis GR, Moraes RR. Intra-radicular dentin treatments and retention of fiber posts with self-adhesive resin cements. Braz Oral Res 2013;27:14-19.ArticlePubMed
  • 12. Soares LP, Dias KR, de Vasconcellos AB, Sampaio EM, Street A. Effects of different pretreatments on the bond strength of a dual-cure resin core material to various fiber-reinforced composite posts. Eur J Prosthodont Restor Dent 2012;20:41-47.PubMed
  • 13. Melo MA, Moysés MR, Santos SG, Alcântara CE, Ribeiro JC. Effects of different surface treatments and accelerated artificial aging on the bond strength of composite resin repairs. Braz Oral Res 2011;25:485-491.ArticlePubMed
  • 14. Moncada G, Angel P, Fernandez E, Alonso P, Martin J, Gordan VV. Bond strength evaluation of nanohybrid resin-based composite repair. Gen Dent 2012;60:230-234.PubMed
  • 15. Hannig C, Laubach S, Hahn P, Attin T. Shear bond strength of repaired adhesive filling materials using different repair procedures. J Adhes Dent 2006;8:35-40.PubMed
  • 16. Fawzy AS, El-Askary FS, Amer MA. Effect of surface treatments on the tensile bond strength of repaired water-aged anterior restorative micro-fine hybrid resin composite. J Dent 2008;36:969-976.ArticlePubMed
  • 17. Gerth HU, Dammaschke T, Züchner H, Schäfer E. Chemical analysis and bonding reaction of RelyX Unicem and Bifix composites-a comparative study. Dent Mater 2006;22:934-941.ArticlePubMed
  • 18. Ferracane JL, Stansbury JW, Burke FJ. Self-adhesive resin cements-chemistry, properties and clinical considerations. J Oral Rehabil 2011;38:295-314.ArticlePubMed
  • 19. Monticelli F, Osorio R, Mazzitelli C, Ferrari M, Toledano M. Limited decalcification/diffusion of self-adhesive cements into dentin. J Dent Res 2008;87:974-979.ArticlePubMedPDF
  • 20. Al-Assaf K, Chakmakchi M, Palaghias G, Karanika-Kouma A, Eliades G. Interfacial characteristics of adhesive luting resins and composites with dentine. Dent Mater 2007;23:829-839.ArticlePubMed
  • 21. Zorzin J, Petschelt A, Ebert J, Lohbauer U. pH neutralization and influence on mechanical strength in self-adhesive resin luting agents. Dent Mater 2012;28:672-679.ArticlePubMed
  • 22. Madruga FC, Ogliari FA, Ramos TS, Bueno M, Moraes RR. Calcium hydroxide, pH-neutralization and formulation of model self-adhesive resin cements. Dent Mater 2013;29:413-418.ArticlePubMed
  • 23. Foxton RM, Nakajima M, Hiraishi N, Kitasako Y, Tagami J, Nomura S, Miura H. Relationship between ceramic primer and ceramic surface pH on the bonding of dual-cure resin cement to ceramic. Dent Mater 2003;19:779-789.ArticlePubMed
  • 24. Matinlinna JP, Lassila LV, Ozcan M, Yli-Urpo A, Vallittu PK. An introduction to silanes and their clinical applications in dentistry. Int J Prosthodont 2004;17:155-164.PubMed
  • 25. Loomans BA, Cardoso MV, Roeters FJ, Opdam NJ, De Munck J, Huysmans MC, Van Meerbeek B. Is there one optimal repair technique for all composites? Dent Mater 2011;27:701-709.ArticlePubMed
  • 26. Blatz MB, Phark JH, Ozer F, Mante FK, Saleh N, Bergler M, Sadan A. In vitro comparative bond strength of contemporary self-adhesive resin cements to zirconium oxide ceramic with and without air-particle abrasion. Clin Oral Investig 2010;14:187-192.ArticlePubMedPDF

Citations

Citations to this article as recorded by  
  • An Innovative Method of Permanent Retention on Veneered Crowns
    Yugandhar Garlapati, Sampath Krishna Veni, Jashva Vamsi Kogila, Polisetty Siva Krishna, K. N. Anand Kumar
    Journal of Indian Orthodontic Society.2025;[Epub]     CrossRef
  • Influence of mechanochemical treatment and oxygen inhibited layer on the adhesion of self-adhesive resin cement to bulk-fill composite resin
    Sreya Dutta, Samikhya Priyadarsani Sahu, Anushka Arora, Srikant Natarajan, Abhishek Parolia, Manuel Thomas
    Cumhuriyet Dental Journal.2024; 27(2): 79.     CrossRef
  • Substrate Rigidity Effect on CAD/CAM Restorations at Different Thicknesses
    César Rogério Pucci, Ana Paula Valente Pinho Mafetano, Alexandre Luiz Souto Borges, Guilherme Schmitt de Andrade, Amanda Maria de Oliveira Dal Piva, Cornelis J. Kleverlaan, João Paulo Mendes Tribst
    European Journal of Dentistry.2023; 17(04): 1020.     CrossRef
  • Microgap Formation between a Dental Resin-Matrix Computer-Aided Design/Computer-Aided Manufacturing Ceramic Restorative and Dentin after Various Surface Treatments and Artificial Aging
    Alexandros Galanopoulos, Dimitrios Dionysopoulos, Constantinos Papadopoulos, Petros Mourouzis, Kosmas Tolidis
    Applied Sciences.2023; 13(4): 2335.     CrossRef
  • Dental Luting Cements: An Updated Comprehensive Review
    Artak Heboyan, Anna Vardanyan, Mohmed Isaqali Karobari, Anand Marya, Tatevik Avagyan, Hamid Tebyaniyan, Mohammed Mustafa, Dinesh Rokaya, Anna Avetisyan
    Molecules.2023; 28(4): 1619.     CrossRef
  • Effect of full-step versus simplified resin cement luting strategies on the push-out bond strength of indirect resin composite restorations bonded to dentin
    Bianca Cristina Dantas da Silva, Isabelle Helena Gurgel de Carvalho, Taciana Emília Leite Vila-Nova, Gabriela Monteiro de Araújo, Boniek Castillo Dutra Borges, Marília Regalado Galvão Rabelo Caldas, Isauremi Vieira de Assunção, Mutlu Özcan, Rodrigo Othávi
    Journal of Adhesion Science and Technology.2023; 37(24): 3552.     CrossRef
  • Effect of various polymerization protocols on the cytotoxicity of conventional and self-adhesive resin-based luting cements
    Ece Irem Oguz, Ufuk Hasanreisoglu, Sadullah Uctasli, Mutlu Özcan, Mehmet Kiyan
    Clinical Oral Investigations.2020; 24(3): 1161.     CrossRef
  • Repair bond strength of resin composite to three aged CAD/CAM blocks using different repair systems
    Pinar Gul, Latife Altınok-Uygun
    The Journal of Advanced Prosthodontics.2020; 12(3): 131.     CrossRef
  • Evaluation of the Surface Characteristics of Dental CAD/CAM Materials after Different Surface Treatments
    Konstantinos Papadopoulos, Kimon Pahinis, Kyriaki Saltidou, Dimitrios Dionysopoulos, Effrosyni Tsitrou
    Materials.2020; 13(4): 981.     CrossRef
  • Adhesive Systems Used in Indirect Restorations Cementation: Review of the Literature
    Cristian Abad-Coronel, Belén Naranjo, Pamela Valdiviezo
    Dentistry Journal.2019; 7(3): 71.     CrossRef
  • Effects of different etching methods and bonding procedures on shear bond strength of orthodontic metal brackets applied to different CAD/CAM ceramic materials
    S. Kutalmış Buyuk, Ahmet Serkan Kucukekenci
    The Angle Orthodontist.2018; 88(2): 221.     CrossRef
  • Ceramic repairs with resins: silanization protocols
    Teresa Cristina Vasconcelos dos Santos
    Journal of Dental Health, Oral Disorders & Therapy.2018;[Epub]     CrossRef
  • Influence of different surface treatments on bond strength of novel CAD/CAM restorative materials to resin cement
    Meltem Bektaş Kömürcüoğlu, Elçin Sağırkaya, Ayça Tulga
    The Journal of Advanced Prosthodontics.2017; 9(6): 439.     CrossRef
  • Adhesive bonding to polymer infiltrated ceramic
    Judith SCHWENTER, Fredy SCHMIDLI, Roland WEIGER, Jens FISCHER
    Dental Materials Journal.2016; 35(5): 796.     CrossRef
  • Orthodontic bracket bonding to glazed full-contour zirconia
    Ji-Young Kwak, Hyo-Kyung Jung, Il-Kyung Choi, Tae-Yub Kwon
    Restorative Dentistry & Endodontics.2016; 41(2): 106.     CrossRef
  • Effect of Silanization on Microtensile Bond Strength of Different Resin Cements to a Lithium Disilicate Glass Ceramic
    Cristina Parise Gré, Renan C de Ré Silveira, Shizuma Shibata, Carlo TR Lago, Luiz CC Vieira
    The Journal of Contemporary Dental Practice.2016; 17(2): 149.     CrossRef
  • Effects of air abrasion with alumina or glass beads on surface characteristics of CAD/CAM composite materials and the bond strength of resin cements
    ARAO Nobuaki, YOSHIDA Keiichi, SAWASE Takashi
    Journal of Applied Oral Science.2015; 23(6): 629.     CrossRef
  • Resin cement to indirect composite resin bonding: Effect of various surface treatments
    Omer Kirmali, Cagatay Barutcugil, Osman Harorli, Alper Kapdan, Kursat Er
    Scanning.2015; 37(2): 89.     CrossRef
  • Impact of different adhesives on work of adhesion between CAD/CAM polymers and resin composite cements
    Christine Keul, Manuel Müller-Hahl, Marlis Eichberger, Anja Liebermann, Malgorzata Roos, Daniel Edelhoff, Bogna Stawarczyk
    Journal of Dentistry.2014; 42(9): 1105.     CrossRef
  • Effect of Plasma Deposition Using Low-Power/Non-thermal Atmospheric Pressure Plasma on Promoting Adhesion of Composite Resin to Enamel
    Geum-Jun Han, Jae-Hoon Kim, Sung-No Chung, Bae-Hyeock Chun, Chang-Keun Kim, Byeong-Hoon Cho
    Plasma Chemistry and Plasma Processing.2014; 34(4): 933.     CrossRef
  • Bonding efficacy of a self-adhesive resin cement to enamel and dentin
    Linhu Wang, Haixing Xu, Songyang Li, Bin Shi, Rong Li, Mingfu Ye, Jing Yang
    Journal of Wuhan University of Technology-Mater. Sci. Ed..2014; 29(6): 1307.     CrossRef
CanvasJS.com
CanvasJS.com
CanvasJS.com

  • ePub LinkePub Link
  • Cite
    CITE
    export Copy Download
    Close
    Download Citation
    Download a citation file in RIS format that can be imported by all major citation management software, including EndNote, ProCite, RefWorks, and Reference Manager.

    Format:
    • RIS — For EndNote, ProCite, RefWorks, and most other reference management software
    • BibTeX — For JabRef, BibDesk, and other BibTeX-specific software
    Include:
    • Citation for the content below
    Bond strength of self-adhesive resin cements to composite submitted to different surface pretreatments
    Restor Dent Endod. 2014;39(1):12-16.   Published online January 20, 2014
    Close
  • XML DownloadXML Download
Bond strength of self-adhesive resin cements to composite submitted to different surface pretreatments
Bond strength of self-adhesive resin cements to composite submitted to different surface pretreatments

Composition of the self-adhesive resin cements tested

*As provided by the manufacturers.

Means (standard deviations) for microshear bond strength, MPa

Distinct lowercase letters in the same column indicate differences between pre-treatments; distinct uppercase letters in the same line indicate differences between resin cements (p < 0.05).

Table 1 Composition of the self-adhesive resin cements tested

*As provided by the manufacturers.

Table 2 Means (standard deviations) for microshear bond strength, MPa

Distinct lowercase letters in the same column indicate differences between pre-treatments; distinct uppercase letters in the same line indicate differences between resin cements (p < 0.05).